- Copper Wire Turns Red or Black After Drawing
Possible Causes:
Drawing fluid pH is too low (< 8.0)
Insufficient BTA concentration
Corrective Actions:
Increase the pH by adding TEA, then replenish BTA as required.
- Sedimentation and Nozzle Blockage
Possible Causes:
BTA may precipitate at the bottom of the system due to insufficient solubility.
Corrective Actions:
Pre-dissolve BTA using TEA and hot water to prepare a concentrate before adding it to the wire drawing system.
- Drawing Fluid Odor and Loss of Corrosion Protection
Possible Causes:
Bacterial growth in water-based drawing fluids may lower the pH value and reduce corrosion protection performance.
Corrective Actions:
Monitor pH regularly and use an appropriate biocide together with TEA supplementation when necessary.
- Localized Pitting Corrosion on Copper Wire Surface
Possible Causes:
Poor water quality used for make-up water or solution preparation. Chloride ions (Cl⁻) in hard water may damage the protective film.
Corrective Actions:
Use deionized water (DI water) or purified water when preparing concentrates and replenishing the wire drawing system.